6150 steel heat treatment
Vanadium spring steel for valve springs, torsion bars and tough tooling. Fine grained by design. Typical practice for AISI 6150: austenitize at 845 to 885 °C (1555 to 1625 °F), quench (oil), then temper at 400 to 540 °C (750 to 1005 °F).
- Austenitize
- 845 to 885 °C
- 1555 to 1625 °F
- Temper
- 400 to 540 °C
- 750 to 1005 °F
- Quench
- Oil
- Typical hardness
- 42 to 48 HRC at spring tempers
The vanadium spec is a 0.15 minimum; the range shown is typical. Vanadium carbides pin grain growth, so it tolerates the hotter end of the austenitizing window.
Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
6150 chemical composition
| Element | Symbol | Weight % |
|---|---|---|
| Carbon | C | 0.48 to 0.53 |
| Manganese | Mn | 0.7 to 0.9 |
| Silicon | Si | 0.15 to 0.35 |
| Chromium | Cr | 0.8 to 1.1 |
| Vanadium | V | 0.15 to 0.25 |
These are the limits of the standard's chemical range. Cr-V spring steel. Also known as: 51CrV4, 1.8159, En47, 735A51.
6150 critical temperatures
| Temperature | What it means | Estimate | Equation |
|---|---|---|---|
| Ac1 | Lower critical temperature | about 738 °C (1360 °F) | Ac1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W |
| Ac3 | Upper critical temperature | about 798 °C (1468 °F) | Ac3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W |
| Ms | Martensite start | about 290 °C (553 °F) | Ms = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo |
Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.
Questions
- What temperature do you harden 6150 steel at?
- Austenitize 6150 at 845 to 885 °C (1555 to 1625 °F), then quench: oil. This is typical published practice; section size and furnace accuracy shift the right number.
- What temperature do you temper 6150 at?
- Temper 6150 at 400 to 540 °C (750 to 1005 °F). Typical hardness: 42 to 48 HRC at spring tempers.
- What do you quench 6150 steel in?
- Oil. The vanadium spec is a 0.15 minimum; the range shown is typical. Vanadium carbides pin grain growth, so it tolerates the hotter end of the austenitizing window.
- What is 6150 steel equivalent to?
- Other designations for 6150, or for its nearest equivalent where marked "near": 51CrV4, 1.8159, En47, 735A51. Check the chemistry on your supplier's datasheet before treating them as the same steel.
Other alloy steels
- 4130Cr-Mo alloy steel
- 4140Cr-Mo alloy steel
- 4340Ni-Cr-Mo alloy steel
- 5160Cr spring steel
- 8620Case-hardening alloy steel
- 9260Si-Mn spring steel
- 9310Case-hardening alloy steel
- 52100Bearing steel
- 80CrV2Cr-V high carbon steel
- 300MUltra-high-strength steel
Sources for this grade: SAE J404 chemical ranges (V is specified as a minimum); Typical published practice.
Enter your own composition and get the numbers, with sources.