A2 vs S7 steel
A2 (Air-hardening tool steel). Air-hardening die steel: the stability of a gas quench with real wear resistance. A fine hard-use knife steel.
S7 (Shock-resisting tool steel). The jackhammer-bit steel: built to take impact at 54 to 57 HRC without shattering.
How A2 and S7 differ
- A2 carries more carbon: 0.95 to 1.05% against 0.45 to 0.55% in S7.
- A2 is alloyed with vanadium (0.15 to 0.5%), which S7 does not have in any real amount.
- A2 has far more chromium: 4.75 to 5.5% against 3 to 3.5%.
- Both are austenitized in much the same range: 925 to 980 °C for A2 and 925 to 955 °C for S7.
- The quench differs. A2: still air or aluminium plates. S7: air up to about 60 mm, otherwise interrupted oil.
Side by side
| A2 | S7 | |
|---|---|---|
| Type | Air-hardening tool steel | Shock-resisting tool steel |
| Carbon (C), wt % | 0.95 to 1.05 | 0.45 to 0.55 |
| Manganese (Mn), wt % | 1 max | 0.2 to 0.9 |
| Silicon (Si), wt % | 0.5 max | 0.2 to 1 |
| Chromium (Cr), wt % | 4.75 to 5.5 | 3 to 3.5 |
| Molybdenum (Mo), wt % | 0.9 to 1.4 | 1.3 to 1.8 |
| Vanadium (V), wt % | 0.15 to 0.5 | none listed |
| Austenitize | 925 to 980 °C (1695 to 1795 °F) | 925 to 955 °C (1695 to 1750 °F) |
| Quench | Still air or aluminium plates | Air up to about 60 mm, otherwise interrupted oil |
| Temper | 175 to 230 °C (345 to 445 °F) | 205 to 540 °C (400 to 1005 °F) |
| Typical hardness | 57 to 62 HRC | 54 to 57 HRC at a 205 C temper |
| Ac1 (lower critical temperature) | Withheld | about 790 °C (1453 °F) |
| Ac3 (upper critical temperature) | Withheld | about 842 °C (1548 °F) |
| Ms (martensite start) | Withheld | about 260 °C (500 °F) |
Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
Heat treating each one
A2
Wrap in stainless foil against decarburization, soak 20 to 45 minutes, cool in still air. Double tempering is standard practice. Distortion is low enough to harden finished parts.
S7
Air hardening in most sections, which keeps distortion down on chisels and punches. Temper immediately after the quench; shock steels resent waiting around untempered.
Questions
- What is the difference between A2 and S7 steel?
- A2 carries more carbon: 0.95 to 1.05% against 0.45 to 0.55% in S7. A2 is alloyed with vanadium (0.15 to 0.5%), which S7 does not have in any real amount.
- Is A2 or S7 harder after heat treatment?
- Typical hardness for A2: 57 to 62 HRC. For S7: 54 to 57 HRC at a 205 C temper. The result depends on the temper you choose.
- Can I heat treat A2 and S7 the same way?
- No, each has its own recipe. A2: austenitize at 925 to 980 °C, quench in still air or aluminium plates, temper at 175 to 230 °C. S7: austenitize at 925 to 955 °C, quench in air up to about 60 mm, otherwise interrupted oil, temper at 205 to 540 °C.
Heat treatment numbers for your own steel, with sources.
Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat