S7 steel heat treatment
The jackhammer-bit steel: built to take impact at 54 to 57 HRC without shattering. Typical practice for S7: austenitize at 925 to 955 °C (1695 to 1750 °F), quench (air up to about 60 mm, otherwise interrupted oil), then temper at 205 to 540 °C (400 to 1005 °F).
- Austenitize
- 925 to 955 °C
- 1695 to 1750 °F
- Temper
- 205 to 540 °C
- 400 to 1005 °F
- Quench
- Air up to about 60 mm, otherwise interrupted oil
- Typical hardness
- 54 to 57 HRC at a 205 C temper
Air hardening in most sections, which keeps distortion down on chisels and punches. Temper immediately after the quench; shock steels resent waiting around untempered.
Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
S7 chemical composition
| Element | Symbol | Weight % |
|---|---|---|
| Carbon | C | 0.45 to 0.55 |
| Manganese | Mn | 0.2 to 0.9 |
| Silicon | Si | 0.2 to 1 |
| Chromium | Cr | 3 to 3.5 |
| Molybdenum | Mo | 1.3 to 1.8 |
These are the limits of the standard's chemical range. Shock-resisting tool steel. Also known as: 1.2355 (near), 50CrMoV13-15 (near).
S7 critical temperatures
| Temperature | What it means | Estimate | Equation |
|---|---|---|---|
| Ac1 | Lower critical temperature | about 790 °C (1453 °F) | Ac1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W |
| Ac3 | Upper critical temperature | about 842 °C (1548 °F) | Ac3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W |
| Ms | Martensite start | about 260 °C (500 °F) | Ms = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo |
Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.
Questions
- What temperature do you harden S7 steel at?
- Austenitize S7 at 925 to 955 °C (1695 to 1750 °F), then quench: air up to about 60 mm, otherwise interrupted oil. This is typical published practice; section size and furnace accuracy shift the right number.
- What temperature do you temper S7 at?
- Temper S7 at 205 to 540 °C (400 to 1005 °F). Typical hardness: 54 to 57 HRC at a 205 C temper.
- What do you quench S7 steel in?
- Air up to about 60 mm, otherwise interrupted oil. Air hardening in most sections, which keeps distortion down on chisels and punches. Temper immediately after the quench; shock steels resent waiting around untempered.
- What is S7 steel equivalent to?
- Other designations for S7, or for its nearest equivalent where marked "near": 1.2355 (near), 50CrMoV13-15 (near). Check the chemistry on your supplier's datasheet before treating them as the same steel.
Other tool steels
- W1Water-hardening tool steel
- O1Oil-hardening tool steel
- A2Air-hardening tool steel
- D2High-carbon high-chromium tool steel
- H13Hot-work tool steel
- M2High-speed steel
Sources for this grade: ASTM A681 chemical ranges; Typical published practice.
Enter your own composition and get the numbers, with sources.