4130 steel heat treatment
Chromoly. The weldable aircraft-tube and roll-cage steel, used normalized or quenched and tempered. Typical practice for AISI 4130: austenitize at 855 to 885 °C (1570 to 1625 °F), quench (oil, water for heavy sections), then temper at 400 to 565 °C (750 to 1050 °F).
- Austenitize
- 855 to 885 °C
- 1570 to 1625 °F
- Temper
- 400 to 565 °C
- 750 to 1050 °F
- Quench
- Oil, water for heavy sections
- Typical hardness
- 28 to 36 HRC quenched and tempered
The low carbon keeps welds tolerable, but thick or restrained joints still deserve preheat. Normalize at 870 to 925 C after welding when the design allows.
Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
4130 chemical composition
| Element | Symbol | Weight % |
|---|---|---|
| Carbon | C | 0.28 to 0.33 |
| Manganese | Mn | 0.4 to 0.6 |
| Silicon | Si | 0.15 to 0.35 |
| Chromium | Cr | 0.8 to 1.1 |
| Molybdenum | Mo | 0.15 to 0.25 |
These are the limits of the standard's chemical range. Cr-Mo alloy steel. Also known as: 25CrMo4, 1.7218, SCM420 (near), En20 (loose).
4130 critical temperatures
| Temperature | What it means | Estimate | Equation |
|---|---|---|---|
| Ac1 | Lower critical temperature | about 741 °C (1366 °F) | Ac1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W |
| Ac3 | Upper critical temperature | about 815 °C (1500 °F) | Ac3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W |
| Ms | Martensite start | about 382 °C (719 °F) | Ms = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo |
Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.
Questions
- What temperature do you harden 4130 steel at?
- Austenitize 4130 at 855 to 885 °C (1570 to 1625 °F), then quench: oil, water for heavy sections. This is typical published practice; section size and furnace accuracy shift the right number.
- What temperature do you temper 4130 at?
- Temper 4130 at 400 to 565 °C (750 to 1050 °F). Typical hardness: 28 to 36 HRC quenched and tempered.
- What do you quench 4130 steel in?
- Oil, water for heavy sections. The low carbon keeps welds tolerable, but thick or restrained joints still deserve preheat. Normalize at 870 to 925 C after welding when the design allows.
- What is 4130 steel equivalent to?
- Other designations for 4130, or for its nearest equivalent where marked "near": 25CrMo4, 1.7218, SCM420 (near), En20 (loose). Check the chemistry on your supplier's datasheet before treating them as the same steel.
Other alloy steels
- 4140Cr-Mo alloy steel
- 4340Ni-Cr-Mo alloy steel
- 5160Cr spring steel
- 6150Cr-V spring steel
- 8620Case-hardening alloy steel
- 9260Si-Mn spring steel
- 9310Case-hardening alloy steel
- 52100Bearing steel
- 80CrV2Cr-V high carbon steel
- 300MUltra-high-strength steel
Sources for this grade: SAE J404 chemical ranges; Typical published practice.