1084 vs 80CrV2 steel
1084 (High-carbon steel). The classic beginner blade steel: eutectoid carbon, wide forgiving windows, clean results in a home shop.
80CrV2 (Cr-V high carbon steel). European chopper steel: 1080 with a little chromium and vanadium for deeper hardening and finer grain.
How 1084 and 80CrV2 differ
- 1084 carries more carbon: 0.8 to 0.93% against 0.75 to 0.85% in 80CrV2.
- 80CrV2 is alloyed with chromium (0.4 to 0.6%), which 1084 does not have in any real amount.
- Both are austenitized in much the same range: 800 to 830 °C for 1084 and 800 to 840 °C for 80CrV2.
- Both are quenched the same way: fast oil.
Side by side
| 1084 | 80CrV2 | |
|---|---|---|
| Type | High-carbon steel | Cr-V high carbon steel |
| Carbon (C), wt % | 0.8 to 0.93 | 0.75 to 0.85 |
| Manganese (Mn), wt % | 0.6 to 0.9 | 0.3 to 0.5 |
| Silicon (Si), wt % | none listed | 0.15 to 0.35 |
| Chromium (Cr), wt % | none listed | 0.4 to 0.6 |
| Vanadium (V), wt % | none listed | 0.15 to 0.25 |
| Austenitize | 800 to 830 °C (1470 to 1525 °F) | 800 to 840 °C (1470 to 1545 °F) |
| Quench | Fast oil | Fast oil |
| Temper | 175 to 230 °C (345 to 445 °F) | 175 to 230 °C (345 to 445 °F) |
| Typical hardness | 57 to 60 HRC after a 190 to 200 C temper | 56 to 60 HRC after a 200 C temper |
| Ac1 (lower critical temperature) | about 715 °C (1319 °F) | about 734 °C (1354 °F) |
| Ac3 (upper critical temperature) | Withheld | about 760 °C (1401 °F) |
| Ms (martensite start) | about 150 °C (303 °F) | about 182 °C (360 °F) |
Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
Heat treating each one
1084
At eutectoid carbon everything transforms cleanly with no excess carbide to manage. Normalize after forging, then harden from a low soak. Pattern-welds beautifully against 15N20.
80CrV2
Handles thicker blades than plain 1080 thanks to the chromium. The vanadium keeps grain fine even with forge heats that wander hot.
Questions
- What is the difference between 1084 and 80CrV2 steel?
- 1084 carries more carbon: 0.8 to 0.93% against 0.75 to 0.85% in 80CrV2. 80CrV2 is alloyed with chromium (0.4 to 0.6%), which 1084 does not have in any real amount.
- Is 1084 or 80CrV2 harder after heat treatment?
- Typical hardness for 1084: 57 to 60 HRC after a 190 to 200 C temper. For 80CrV2: 56 to 60 HRC after a 200 C temper. The result depends on the temper you choose.
- Can I heat treat 1084 and 80CrV2 the same way?
- No, each has its own recipe. 1084: austenitize at 800 to 830 °C, quench in fast oil, temper at 175 to 230 °C. 80CrV2: austenitize at 800 to 840 °C, quench in fast oil, temper at 175 to 230 °C.